Translate

Blog Archive

Tuesday, January 4, 2022

Stainless Steel 405 (UNS S40500)

wilsonpipeline Stainless inventory includes Alloy 405 (UNS S40500) in  Stainless Steel Pipes.  Other product forms such as Stainless Steel FlangesStainless Steel Pipe Fittings.

Overview


General Properties

Alloy 405 is a 12% chromium stainless steel designed to be used in the as-welded condition. Unlike the other grades of 12% chromium stainless, 405 is not vulnerable to extensive hardening through air cooling from high temperatures.

Specifications: UNS S40500

Applications:

Applications that frequently use alloy 405 include, but are not limited to:

  • Steam nozzles
  • Partitions
  • Annealing boxes
  • Quenching racks
  • Fabrications that cannot be annealed after welding

 

Standards:

  • ASTM/ASME: UNS S40500
  • EURONORM: FeMi35Cr20Cu4Mo2
  • DIN: 2.4660

Resistance

Corrosion Resistance

  • Same corrosion resistance of Type 410 Steel
  • Used in situations where more weldability is desired than Type 410

Processing

Machinability

  • Type 405 can be easily machined due to its soft and ductile characteristics

 Weldability

  • Can be welded using shielded fusion and resistance techniques
  • Oxyacetylene is not recommended
  • Post weld annealing will maximize ductility

Properties

Chemical Properties:

CCrFeMnSiSPNiAl
4050.08 max

min: 11.5
max: 14.5

balance

1.0
max

1.0
max
0.03
max

0.04
max

0.50
max

min: 0.1
max: 0.3

Mechanical Properties:

GradeTensile Strength ksi (MPa) minYield Strength 0.2% offset ksi (MPa) minElongation (% in 50mm) minHardness (Brinell) MAXHardness (Rockwell B) MAX
405

60
(415)

25
(170)

20

179

88

Physical Properties:

Denstiy
lbm/in3
Coefficient of
Thermal Expansion (min/in)-°F
Thermal Conductivity BTU/hr-ft-°FSpecific Heat BTU/lbm -°FModules of Elasticity (annealed)2-psi
at 68 °Fat 68 – 212°Fat 68 – 1832°Fat 200°Fat 32 – 212°Fin tension (E)
0.2799.220.54160.1128 x 106

0 comments: